Chain Parameters of Amorphous Polymers
Compound |
Me |
C∞ |
νe |
ρa |
PODMA | 225000 | 20.6 | 0.004 | 0.942 |
PODMA | 112000 | 14.1 | 0.008 | 0.93 |
PDMA | 61000 | 13.4 | 0.016 | 0.95 |
PHMA | 33500 | 12.2 | 0.030 | 1.01 |
PtBMA | 28300 | 12.0 | 0.036 | 1.02 |
PCHMA | 34700 | 11.6 | 0.032 | 1.10 |
PS | 16600 | 10.3 | 0.064 | 1.06 |
PαMS | 16400 | 10.1 | 0.065 | 1.07 |
PVAc | 9700 | 9.4 | 0.123 | 1.19 |
PEA | 8200 | 9.3 | 0.137 | 1.12 |
PMA | 9100 | 8.3 | 0.122 | 1.22 |
PMMA | 11300 | 8.1 | 0.101 | 1.15 |
PEMA | 8600 | 8.0 | 0.130 | 1.12 |
PEI | 4950 | 7.8 | 0.270 | 1.34 |
PVC | 4200 | 7.6 | 0.259 | 1.38 |
POM | 2600 | 7.5 | 0.479 | 1.23 |
PE | 1400 | 6.9 | 0.607 | 0.85 |
PEO | 1900 | 6.9 | 0.598 | 1.13 |
N6 | 2500 | 6.2 | 0.436 | 1.08 |
N66 | 2000 | 6.1 | 0.537 | 1.08 |
PP | 4600 | 6.0 | 0.187 | 1.86 |
PET | 1450 | 4.1 | 0.919 | 1.33 |
TMPC | 3400 | 3.1 | 0.315 | 1.08 |
PPO | 3600 | 3.0 | 0.298 | 1.06 |
PC | 1900 | 2.4 | 0.626 | 1.21 |
PSO | 2300 | 2.2 | 0.535 | 1.24 |